Copper plating is attracting attention in silicon heterojunction (HJT) solar cells because it can reduce reliance on silver, but the patterning step that defines the plating mask has its own reliability problem. A Chinese research team has traced a gradual efficiency loss in copper-plated HJT cells to wear of the screen mesh used to print photoresist, and has proposed a modified screen design intended to protect the cell’s sensitive passivation layers.
The work, published in Solar Energy, addresses a step that differs from conventional silver-paste screen printing. In silver paste printing, screen openings occupy only 2–5% of the total area and an emulsion layer keeps the mesh from direct contact with the wafer. For full-area photoresist coating, however, the screen typically has no emulsion coverage so that resist can be deposited uniformly across the wafer. The mesh therefore contacts the wafer directly and extensively during every printing cycle, Lang Zhou, the corresponding author, told pv magazine.
That contact matters because HJT cells depend on passivating contacts that are sensitive to mechanical and thermal stress. Prior investigations cited by the researchers found conversion efficiency declining from 26.2% to 25.7% over 15,000 consecutive printing cycles in commercial solar cell production. Open-circuit voltage and fill factor accounted for most of the loss, while short-circuit current density and electrical resistance remained largely unchanged. Minority-carrier lifetime degradation rose from 0.61% with a new screen to 11.0% after 15,000 cycles.
Using three-dimensional confocal microscopy, the team identified progressive wear of the screen mesh knuckles as the main cause. As the knuckles wore down, their contact area with the wafer increased, raising mechanical stress on the underlying passivation layers. Scanning electron microscopy showed no visible surface scratches, but photoluminescence measurements indicated increased recombination losses. The researchers interpret this as evidence of damage to the amorphous silicon/crystalline silicon interface.
A buffer layer with a trade-off
To reduce that damage, the researchers developed an emulsion buffer layer that prevents direct contact between the mesh and the wafer. They evaluated six patterns with emulsion coverage ratios from 2.9% to 16.6%. The results exposed a trade-off: higher emulsion coverage reduced mechanical damage but impaired photoresist coating uniformity and ink distribution. A coverage ratio of 4.7% gave the best balance, limiting minority-carrier lifetime degradation to 0.41% after 10,000 printing cycles while maintaining relatively good coating uniformity.
The improvement is attributed to the emulsion layer blocking direct mesh-to-wafer contact and thereby reducing cumulative mechanical damage to the passivation layers. Zhou described the finding as evidence that a relatively simple modification to screen design can substantially mitigate printing-induced degradation, offering a practical route to improving manufacturing reliability for copper-plated HJT cells.
What the result does and does not show
The data point to a specific failure mode rather than a general penalty from screen printing. Efficiency losses were concentrated in voltage and fill factor, and the microscopy and lifetime measurements connect those losses to mechanical wear at the mesh knuckles. That makes the screen itself an active reliability variable in a process often treated as a patterning step upstream of copper plating.
The proposed buffer does not eliminate degradation. At the best coverage ratio, the reported lifetime degradation after 10,000 cycles was 0.41%, not zero, and the study reports a trade-off with coating uniformity. The mitigation test covered 10,000 cycles, while the earlier production observation covered 15,000, so the two figures describe different test horizons and should not be read as a direct before-and-after comparison. The researchers also describe the approach as potentially improving suitability for large-scale manufacturing, not as a validated commercial fix.
Those boundaries matter for scale-up. A screen modification that protects passivation must still deliver uniform photoresist across the full wafer, because poor coating would undermine the plating mask. The 4.7% coverage result suggests a narrow window: enough emulsion to buffer contact, but not so much that it disrupts resist distribution. The six-pattern range from 2.9% to 16.6% shows why the design needs optimization rather than a blanket increase in emulsion coverage.
Copper metallization’s wider push
The finding arrives as copper metallization draws more attention as a silver-reduction path for HJT. In April 2026, researchers at China’s Nankai University reported a silver-free HJT solar cell with 25.2% efficiency using plasma-induced interface engineering and copper electroplating. That approach addressed adhesion, contact resistance and stability challenges at the indium tin oxide interface.
Separately, scientists at Germany’s Forschungszentrum Jülich achieved 23.08% efficiency in a fully copper-metallized HJT solar cell. The silver-free device showed a relatively small efficiency penalty compared with its silver-metallized counterpart, while cells combining silver-copper paste on the front side with silver contacts on the rear reached 23.95%. Those results underline copper’s potential to reduce silver consumption, while leaving room for further improvements in processing and electrical performance.
For copper-plated HJT, the screen-printing study adds a manufacturing-quality issue to that agenda. The metal stack may be silver-free, but the resist pattern still depends on a mechanical printing process that can damage the cell interface over repeated cycles. Controlling mesh wear and contact stress is therefore part of making copper plating reliable, not merely a peripheral screen-maintenance detail.
The Chinese team’s contribution is to identify the wear mechanism and show a measured mitigation path. Whether a 4.7% emulsion buffer can hold up in high-volume production, across screen lifetimes and coating conditions, remains to be established. The study’s own framing is cautious: the modification may improve manufacturing reliability, but the reported trade-off and test horizon leave room for process optimization.